Checking and reconditioning of crankshaft

WIS 03-318

Checking and reconditioning of crankshaft – rysunek
Checking and reconditioning of crankshaft – rysunek

Data

Fitted bearing Pertinent thickness of thrust washers

2.15

–

2.20

2,25 or

2.35

or

2.40

Permissible out-of-round of crankshaft . 0.005 journals and crankpins

Permissible conicity of crankshaft journals and crankpins .0.01
Permissible radial runout of flywheel flange0.02
Permissible axial runout of fitted bearing0.02
Filletson crankshaft bearing journals2.5 to 3.0
— on crankpinsoe_ __ 3.0 to 3.5
Permissible radial runout of crankshaft journals when mounted on outer journalsjournal Il, V journal Il, 1Vwo0.16 0.25
Scleroscope hardness of crankshaft journals and crankpins55–74
Permissible unbalance of crankshafti5 cmg

Note The bearing journals of crankshaft are not inductance hardened similar to other engines, but are hardened in a nitride bath.

Contrary to inductance hardened crankshaft, a bathnitrided crankshaft is hardened at its entire surface.

Conventional hardness tester (hardness drop tester) provides no information concerning proper hardness (depth of connecting layer) for crankshafts hardened in a nitride bath. No hardness test according to the above method is therefore required.

When testing and reconditioning crankshafts, proceed in sequence of diagram below.

Diagram

* Refer to section ‘Explanations Concerning Diagram”

V = scrap.

Visual checkup Heavy damage? yes Vv

no

Crack test* Cracks showing up? yes Vv

no no

Checking and reconditioning of crankshaft – rysunek

Measuring journals Check whether reginding Dimensions in order ___ no __. within final repair is still

yes yes

Lapping* crankshaft

Dimensional journal (Running concentricity Dimensions

yes test* showing up?___ yes____ V

no

i Completing crankshaft, hardening* balance, if possible

Explanations concerning diagram

Crack test

Clean crankshaft. Bearing journals should be free of oil and grease.

Magnetize crankshaft and apply fluorescent powder (fluxing).

A color penetration test (immersion in bath or using spray can) may also be applied.

Aid: Paint or fluorescent powder Cleaning agent Developer

Hardening

Crankshaft must be nitride-hardened in a salt bath.

Attention! Prior to nitriding, close all threaded bores in crankshaft.

Hardened threads will loose in strength and may therefore break out when tightening screws.

Screw-in necked-down screws on flywheel flange.

Screw-in a hollow center screw M 18 x 1.5 x 45 at front on crankshaft.

Center screw is bored hollow to prevent a chemical reaction in salt bath caused by the air which might be enclosed behind screw.

Duration and bath temperature are shown in nitriding specifications included upon delivery of nitriding equipment.

To avoid distorsion of crankshaft, suspend crankshaft vertically into nitriding bath.

Material data: 49 Mn VS 3 BY 80–95.

Depth of connecting layer: 0.014–0.022 mm.

Then cool crankshaft in oil or salt water to 90° C.

Upon nitriding, remove nitride residue in oil! bores.

Attention! Do not straighten crankshaft anymore after bath nitriding.

Lapping

Lap bearing journals with a lapping belt (grain 400) as follows:

Slowly pre-lap for approx. 5 seconds Lap fast for approx. 25 seconds

Checking of hardness

Check nitrided bearing journals by means of metallographic etching.

Pertinent tests can be made on scrapped crankshafts.

Corrosion protection

Coat crankshafts which are not immediately installed again with engine initial operation oi! (SAE 30).