Checking and reconditioning crankshaft

WIS 03-318

Data

Checking and reconditioning crankshaft – rysunek
Checking and reconditioning crankshaft – rysunek

Crankshaft, Thrust bearnormal size Crankshaft ings width of Corresponding and repair journal dia. flanged shell thrust washer stages bearings thickness

69.96 Normal size . _——33.80 ——2.15 ee
69.9633.902.20

69.71 1st repair stage — 69.70 2.25 69.46 2nd repair stage —_— or 69.45 34.40 —_ Re ee 2.35 69.21 34.60 3rd repair stage basic or 69.20 2.40 4th repair stage 68.96. 68.95

Permissible ovality of crankshaft journals and crankpins0.005
Permissible conicity of crankshaft journals and crankpins0.01
Permissible wobble of thrust bearing0.02
Permissible eccentricity of flywheel flange0.02
Fillets on crankshaft journals and crankpin3.0 to 3.5
616Journals It, IV0.07
Permissible eccentricity of crankshaft journals,Engines 615,Journal tI0.10
mounted at outer journalsoo 617ee Journals II, V0.07
Engineaa Journals Il, 1V: = 0.10
Scleroscope hardness of crank-as new74–84
shaft journals and crankpins Permissible unbalance of crankshafta tolerance limit60?) 15 cmg

1) Figures when using thrust washers. When using flanged shell bearings: journal width = 34.00–34.60 mm. At least 2/3 of the pin/journal circumference must show tolerance limit.

Special tool

Drop hardness tester – 000 589 20 21 00

Note For checking and reconditioning crankshafts proceed in the order of the overleaf diagram.

Diagram

*See section “Explanations to diagram”.

V = Discard.

Heavy damage? yes

no

Crack check * Cracks to be seen? yes _

no

Hardness test * ~~ no All pins/journals Scleroscope hardness at least 60 around 2/3 of circumference

yes

Pin/journal measurement Values satisfied? _. no Check no whether no regrinding yes is still yes possible within Hardening* _ _

Lapping

repair stage 4 Pins/journals withPins/journals with Dimension check out fillet hardening fillet hardening Values satisfied? no

___ yes Induction yes hardening, equipment Fit out Straighten available? = Induction or flame hardening crankshaft crankshaft; balance if possible no yes

Grind

crankshaft

Check hardness Crack check InducCracks tobefound? __ yes Vv tion

by etching *

hardening

Stress-relieve no crankshaft at 80/C

for 2 hours

See lapping

See crankshaft straightening

Crack check

Clean crankshaft, making sure that pins and journals show no signs of oil or grease. Magnetize crankshaft and apply fluorescent powder (fluxing). It is also possible to employ a paint penetration method (dipping in bath or spraying from can).

Materials: Paint or fluorescent powder, cleaning agent, developer

Checking and reconditioning crankshaft – rysunek

Hardness test

Check hardness using hardness tester (scleroscope hardness).

Minimum hardness of 60 must be obtained around 2/3 of pin/journal diameter.

Checking and reconditioning crankshaft – rysunek

Hardening

Pins/journals without hardened fillets can be treated by induction or flame-hardening. tn contrast, pins/ journals with hardened fillets (arrows) must always be hardened by induction. Failing this, discard crankshaft.

Checking and reconditioning crankshaft – rysunek

For hardening pins/journals not having hardened fillets, be sure to obtain distance A between fillet and end of hardened section (5–6 mm).

To obtain satisfactory hardness, it is essential to adjust the hardening system by means of microsections.

These sections can be taken from hardening experiments on discarded crankshafts.

Check hardening effect by etching pin/journal surface with a 2 % alcohol solution of nitric acid (HNO3).

No dark spots must appear on the pin/journal surface.

The unhardened fillets go dark.

In contrast, the hardened fillets must be as light as the pin/journal surfaces.

To compare the effects it is advisible to etcha metallographically checked pin/journal.

Finally wash off the nitric acid carefully with alcohol.

Corrosion protection

Crankshafts which are not put back immediately must be lubricated with engine oil (SAE 30 runningin oil).