Checking and reconditioning of crankshaft
WIS 03-318
Data
| Crankshaft standard dimension and repair stages | journal |
| Standard dimension | 69.96 69.95 |
| 1st repair stage . 2nd repair stage | 69.71 69.70 69.46 69.45 |
3rd repair stage 69.21 69.20
4th repair stage 68.96 68.95
Permissible out-of-round of crankshaft . 0.005 journals and crankpins
Permissible conicity of crankshaft 0.01 journals and crankpins
Permissible radial runout of 0.02 flywheel flange
Permissible axial runout of 0.02 fitted bearing
illets on cran shaft journals 3 to 32.30 Fillet kshaft j and crankpins
Permissible radial runout of crankshaft Journal Il, 1V 0.07 journals when mounted at outer – – oe journals Journal II] 0.10
Scleroscope hardness of crankshaft When new 74–84 journals and crankpins 1) _ Limit 60
Permissible unbalance of crankshaft
1) The limit value should be available at least at 2/3 of journal and crankpin circumference.
07 2219/4
Special too!
CaS] Impact hardness tester srogk -6290 – 000 589 20 21 00
Note When checking and reconditioning crankshaft, proceed in sequence of diagram below.
Diagram
* Refer to section ‘Explanations concerning diagramm”.
V = Scrap
Visual checkup
Heavy damage? yes _ Vv
no
Crack test* Cracks showing yes V up?
no
Hardness test* _
_ no All bearing journals Scleroscope hardness min. 60 at 2/3 of journal circumference
yes
Measuring journal
Dimensions in order? nO Check whether __ no Vv regrinding – no – —V within final yes repair stage — yes
4 is still
possible Hardening* a
Lapping
Dimensional
Journal with Journal without
checkup
hardened fillets hardened fillets Dimensions in order? ___—s no
Induction yes hardening facilities \ _ available? Inductance or flame Crankshaft hardening
Complete
crankshaft;
straighten
balance, if
no yes
possible
Crankshaft
grind
Induc- Test hardness Crack test tance by etching* Cracks showing up? ____ yes Vv hardening
Relieve crankshaft
no stress at 80° C
for 2 hours
Refer to lapping
Refer to crankshaft,
straighten
Explanations concerning diagram
Crack test
Clean crankshaft. Bearing journals should be free of oil and grease. Magnetize crankshaft and apply fluorescent powder (fluxing). A color penetration test (immersion in bath or using spray can) may also be applied.
Aids: Paint or fluorescent powder, cleaning agent, developer.
Hardness test
Check hardness with impact hardness tester (scleroscope hardness).
A minimum hardness of 60 should prevail at 2/3 of journal circumference.
Hardening
Journals without hardened fillets can be inductance hardened or flame hardened. Journals with hardened fillets (arrows) should be inductance hardened on principle. If this is not possible scrap crankshaft.
When hardening journals without hardened fillets the distance ‘‘A” between runout of hardened surface and fillet (5–6 mm) must be maintained.
Checking the hardening
For perfect hardening, check adjustment of hardening equipment by metallographic grinding.
Pertinent tests can be made on scrapped crankshafts.
Check hardening by etching the journal surface with a 2% alcoholic nitric acid (HNO3) solution.
No dark spots should show up at surface of journal.
Non-hardened fillets will become dark.
The hardened fillets, on the other hand should be as bright as the journal surface.
For comparison, we recommend an etching test on a metallographically inspected journal.
Then, carefully wash off nitric acid by means of alcohol.
Corrosion protection
Coat crankshafts which are not immediately installed again with engine initial operation oil (SAE 30).