Checking and reconditioning crankshaft
WIS 03-318
Preliminary jobs: Crankshaft removed.
P03-0108–53
Crankshaft 2.0… 2.0.2… 000.000. eee eee clean Crack test 2… eee ee eee perform; apply fluorescent powder (magnaflux) or use penetration method. Hardness test (scleroscope hardness) …….. perform with impact hardness tester 000 589 20 21 00. Distance (A = 5-6mm) …………..— when hardening journals without hardened fillets, maintain distance A between hardened runout and fillet radius. dJournalS oe ee eee can be hardened inductively or with flame.
AN Harden journals with hardened fillets (arrows) inductively only.
ei RA03.1024 – 318/1
Crankshaft Crankshaft Fitted bearing Connecting rod normal dimenbearing journal Associated bearing bearing journal sions and repair dia. thickness of dia.
width
stages thrust Width of washers
| Standard dimension | 57.940 57.965 | 2.15 2.20 | 26.52″ 26.50 26.62” 26.60 | 27.96 28.04 | ||
| 1st repair stage | 57.700 57.715 | 26.72″ 26.70 | ||||
| 2nd repair stage | 57.450 57.465 | 2.25 or | or 26.92″ | |||
| 3rd repair stage | 57.200 57.215 | 2.35 or | 26.90 or | — 28.30 | ||
| 4th repair stage | 56.950 56.965 | 2.40 | 27.02″ 27.00 | |||
| 1) Up to 06/84 2) Starting 07/84 Test values | ||||||
| Permissible deviation of crankshaft main and rod journals in mm | 0.005 | |||||
| Permissible conicity of crankshaft main and rod journals in mm | 0.01 | |||||
| Permissible roughness of crankshaft main and rod journals (Ra) in mm | 0.005 — 0.015 | |||||
| Permissible deviation of flywheel flange from true in mm | 0.02 | |||||
| Permissible axial runout of fitted bearing in mm | 0.02 | |||||
| Fillet radii in mm | on crankshaft main journals | 2.5 — 3.0 | ||||
| on rod journals | 3.0 – 3.5 | |||||
| Permissible deviation of crankshaft main journals when mounted in outer crankshaft | Journal Il, IV | 0.16 | ||||
| bearing journals in mm | Journal III | 0.25 | ||||
| Scleroscope hardness of crankshaft main and rod journals | 55–74 | |||||
| Permissible unbalance of crankshaft | 10 cmg | |||||
wale RA03.1024 – 318/2
Special tool
Note When testing and reconditioning crankshafts, proceed in sequence shown in diagram below.
wim RA03.1024 – 318/3
A. Testing, grinding
| Visual check Heavy damage | cay Gamage | |||
| Yes | No | |||
| Scrap | crap | |||
| Vv | ||||
| Crack test ’) Cracks present | racks poser | |||
| Yes | No | |||
| Scrap | crap | |||
| Hardness test ’) All bearing journals Scleroscope hardness min. 55 on 2/3 of journal circumference | ||||
| Yes | No | |||
| see Hardening (section B) | ||||
elite RA03.1024 – 318/4
Yes No
| WV | |||||
| Check whether regrinding is still possible within last specified repair stage 4. | |||||
| Yes | No | ||||
| Scrap | |||||
| vv | |||||
| Grind crankshaft | |||||
| vv | |||||
| Crack test Cracks present | |||||
| Yes | No | ||||
| Vv | Vv Scrap | v | |||
| Lapping Dimension check Dimensions okay | |||||
| Yes | No | ||||
| Vv | |||||
| see Testing/Regrinding | |||||
| Vv | Be | ||||
| Complete crankshaft | rrankshaft | ||||
| Vv | Be | ||||
| End of test | Bn | ||||
wim RA0I.1024 – 318/5
Check whether regrinding is still possible within specified repair stage 4.
Yes No
Scrap
Vv Hardening ’)
Journals with hardened fillets Journals without hardened fillets
| VV | ||||||
| Induction hardening | Induction or flame hardening | |||||
| Facilities available | (LMI GVanaie | |||||
| Scrap | No | |||||
| Vv | ||||||
| Scrap | ||||||
| v | ||||||
| Induction hardening | duction hardening | |||||
| Check hardness by etching ’) | heck hardness by etching ’) – | | |||||
| Vv | ||||||
| Relieve crankshaft at 80 °C, 2 hours | elieve crankshaft at 80 °C, 2 hours | |||||
| v | ||||||
| Check concentricity, dimensions okay? | heck concentricity, dimensions okay? | |||||
Journals with hardened fillets Journals without hardened fillets
| Yes | No | ||
| Scrap | Straighten | ||
Vv Vv
See Grinding crankshaft (section A)
Clean crankshaft. Bearing journals should be free of oil and grease. Magnetize crankshaft and apply fluorescent powder (magnaflux). A color penetration method may also be used (immersion in bath or using spray can).
Agent: Paint or fluorescent powder, cleaning agent, developer
Hardness test
Test hardness with impact hardness tester 000 589 20 21 00 (scleroscope hardness).
The minimum hardness of 55 should be present on 2/3 of journal circumference.
Hardening
Journals without hardened fillets can be hardened inductively or flame-hardened. Journals with hardened fillets (arrows) must always be hardened inductively.
if this is not possible, scrap crankshaft.
P03-0091–13
aie RA03.1024 – 9318/7
To achieve perfect hardening check adjustment of hardening equipment using microsections.
These can be obtained from scrapped crankshafts hardened for testing purposes.
Check hardening by etching the journal surface with a 2 % solution of alcoholic nitric acid (HNO3).
Dark spots should not appear on the journal surface.
Unhardened fillets will become dark.
On the other hand hardened fillets should be as bright as the surface of the journals.
We recommend comparing the etching test with a journal tested via metallographic microsection.
Then carefully wash off nitric acid with alcohol.
Corrosion protection
Crankshafts which are not installed again immediately should be lubricated with engine initial operation oil (SAE 30).