Checking and reconditioning of crankshaft
WIS 03-318
Data
| Crankshaft standard dimension and repair stages | Crankshaft bearing journal diameter | Width of thrust bearing journal | Crank pin diameter | Width of pins | |||||
| Standard dimension | 63.965 63.950 | 27.000 27.021 | 51.965!) 51.945 | 47.9657) – 47.945 | 50.000 50.100 | ||||
| Ist repair stage 2nd repair stage | 63.715 63.700 63.465 Se 63.450 | to 27.50 | 51.7151) 51.695 51.465!) a 51.445 | 47.715?) —— 47.695 47.4657) 47.445 | to 50.30 | ||||
| ae 3rd repair stage | 63.215 63.200 | up | 51.215’) 51.195 | 47.2157) 47.195 | up | ||||
| 4th repair stage | 62.965 62.950 | 50.965′) – 50.945 | 46.9657) 46.945 | ||||||
| Permissible crankshaft journal and crank pin runout | 0.0025 | ||||||||
| Permissible deviation of the connecting rod journal surface axis to the reference axis of the crankshaft journals | and V, from parallel | 0.01 | |||||||
| Permissible radial runout of the rear crankshaft flange? ) | 0.02 | ||||||||
| Permissible axial runout of the rear crankshaft flange° ) | 0.012 | ||||||||
| Permissible axial . crankshaft ” bearing 9) journals? | runout of the | Journals Il, 1V Journals If | 0.07 0.10 | ||||||
| Permissible deviation of the front crankshaft journal‘ ) | from the cylindrical shape | 0.005 | |||||||
| from axial runout? ) | 0.030 | ||||||||
| Permissible deviation of the bearing surfaces of the thrust bearing | f rom radia! dial runo ut?) | 0.02 | |||||||
| Fillet radii at the crankshaft and connecting rod bearing journals | 2.5–3 | ||||||||
| Crankshaft bearing journal diameter front | 31.984–32.000 | ||||||||
| Bearing surface dia. for radial sealing ring rear, ground without helix | 99.928 | ||||||||
| Scleroscope hardness of crankshaft bearing | when new | ||||||||
| journals and crank pins | we limit value | ||||||||
1) Engines 116 and 117 except 2), 2) 116.960/961 SG) CS) Gs —116.962/963 and 117.962/963. With crankshaft resting on outer crankshaft bearing journals and V and one full turn. When measuring in the installed position, eliminate end float by pressing against the crankshaft journal. Limit value should be available at least on 2/3 of journal circumference.
Impact hardness tester (scleroscope) – 000 589 20 21 00
Note
During repair the crankshaft need not be balanced.
When checking and reconditioning the crankshaft proceed according to the following diagram.
Group number for crank pin diameter (standard dimension)
1 = 51.945–51.954 mm and 47.945–47.954 mm 2 = 51.955–51.965 mm and 47.955–47.965 mm
The stamped-in figure at bottom applies to the 1st crank pin.
Diagram
* See section ,,Explanation on diagram”. 1
V = Scrapping.
Visual checkup
Heavy damage? yes
no
Crack test* Cracks present? yes
no
Hardness test* no All bearing journals scleroscope hardness minimum 60 on 2/3 of the journal circumference
yes
Measure pin (journal) Dimensions in order? === no Check whether no Vv regrinding is still no Vv possible yes within last yes specified repair Hardening*
Lapping
stage 4.
Dimensional checkup Journal or pin Journal or pin Dimensions in order? ____ no with hardened without hardened fillets fillets
yes yes Induction hardening Complete Straighten facilities crankshaft crankshaft available? Induction or flame hardening
Grind
no yes crankshaft
Crack test Check hardness InducCracks showing? by etching* yes __Y tion hardening
Relief crankshaft
no
at 80 °C for
2 hours
See Lapping
See Straightening of crankshaft
Explanation of diagram
Crack test
Clean crankshaft. Bearing journals and pins should be free of oil and grease. Magnetise crankshaft and apply fluorescent powder (fluxing). A color penetration method may also be used (immersion in bath or using spray can).
Flux agent: Paint or UV-oil, cleaning agent, developer
Hardness test
Test hardness with impact hardness tester (scleroscope).
The minimum hardness should be available on 2/3 of the journal and pin circumference.
Hardening
Journals and pins without hardened fillets can be inductance hardened or flame hardened. On the other hand, journals and pins with hardened fillets (arrow) must always be inductance hardened. If this is not possible, scrap the crankshaft.
When hardening journals and pins without hardened fillets, the distance A between hardened runout and fillet radius (4–5 mm) must be maintained.
The running surface for the rear radial sealing ring is hardened and ground without helix (previously 60° helix).
For perfect hardening, check adjustment of hardening equipment by means of metallographic etching (grinding).
Pertinent tests can be made with scrapped crankshafts.
Check hardening by etching surface of journals and pins with a 2% solution of alcoholic nitric acid (HNO3).
No dark areas should appear on journal or pin surfaces.
Unhardened fillets will become dark.
Hardened fillets, on the other hand, should be as bright as the surface of pin or journal.
A journal or pin which has already passed metallographic inspection may be used for comparison.
After the test, carefully wash off nitric acid with alcohol.
Corrosion protection
Crankshafts which are not immediately installed again should be lubricated with engine initial operation oil (SAE 30).