Checking and reconditioning of crankshaft

WIS 03-318

Data

Crankshaft standard dimension and repair stagesCrankshaft bearing journal dia.Width of journal at fitted bearingCrankpin dia.Width of pins
Standard dimension63.96 63.9527.00 27.0251.96 51.9550.00 50.12
1st repair stage63.71 63.70ELAR 51.70
2nd repair stage63.46 63.45to 27.5051.46 51.45to 50.30
3rd repair stage 4th repair stage63.21 63.20 62.96. 62.95up– 51.27 51.20 50.96 50.95up

Permissible radial runout of crankshaft journals and crankpins 0.0025

Permissible deviation of surface line of crankpins in relation . . 0.01 to reference axis of crankshaft journals and V, from parallel

Permissible radial runout of rear crankshaft flange?) 0.02

Permissible axial runout of rear crankshaft flange°) 0.012

journal tI, 1V 0.07

Permissible radial runout of crankshaft __

3 journals~ ) journal II 0.10

from cylindrical shape 0.05 Permissible deviation of front crankshaft journal”) —— a radial runout?) 0.03

Permissible deviation of running surfaces of thrust bearing axial runout?) 0.02

Fillets on crankshaft journals and crankpins 2.5-—-3

Crankshaft journal dia. front 31.984–32.000

99.928 Running surface dia. for radial sealing ring rear, ground free of twist —_—— 99.874

value when new 71–81 Scleroscope hardness of crankshaft journals and crankpins limit value 61′)

1 se + : . ) The limit value should be available at least at 2/3 of journal and crankpin circumference. ) When measuring in installed condition, eliminate radial bearing play by pushing against crankshaft journal. ) With crankshaft resting on outer crankshaft bearing journal and V and at one full turn.

Checking and reconditioning of crankshaft – rysunek

The differenciating characteristics of crankshafts of engines 116 and 117 are shown on drawing and in table. 1 Lam, Starting with installation of transmission 722.3 = X 4

(W 4 A 040) into model 107.026 the crankshaft of —E engine 117.960 is standardized with that of engine Gp 117.961.

Crankshafts engines 116 and 117

Checking and reconditioning of crankshaft – rysunek

together with a length compensating washer, part no. 116 032 03 76, (10.5 mm thick) and the longer (29 mm, up to now 23 mm) necked-down screws, part no. 116 032 04 71.

Special tool

Checking and reconditioning of crankshaft – rysunek

Hardness tester (Scleroscope) CS ae – 000 589 20 21 00

Note Following repairs, no balancing of crankshaft is required.

When checking and reconditioning crankshaft, proceed in sequence of diagram below.

Group number for crankpin dia. (standard dimension)

1 = 51.945–51.954 mm or 47.945–47.954 mm 2 = 51.995–51.965 mm or 47.955–47.965 mm

The number punched in at bottom applies to 1st crankpin.

Diagram

* Refer to section ‘Explanations concerning diagram”.

V = scrap.

Visual checkup Vv Heavy damage? yes

no

Crack test* Vv Cracks showing up? yes

no

Hardness test* no All bearing journals Scleroscope hardness min. 60 at 2/3 of journal circumference

yes

Measuring journal

Dimensions in order? — = no

Check whether

no Vv no Vv

regrinding

within final yes repair stage 4 yes

is still possible

Hardening*

Lapping

Journal without Journal with hardened hardened

Dimensional checkup

fillets fillets

Dimensions in order? —— no

Induction yes yes hardening facilities available?

Straighten

Complete

Inductance or crankshaft crankshaft flame hardening no yes

Grind

crankshaft

Test hardeness Induction Crack test

by etching*

hardenCracks yes ——V ing showing up?

Relieve crank-

shaft stress

at 80 °C for

2 hours

Refer to lapping

Refer to

straightening

of crankshaft

Explanations concerning diagram

Crack test

Clean crankshaft. Journals should be free of oil and grease. Magnetize crankshaft and apply fluorescent powder (fluxing). A color penetration test (immersion in bath or using spray can) can also be applied.

Checking and reconditioning of crankshaft – rysunek

Aids: Paint or UV-oil, cleaning agent, developer

Hardness test

Check hardness with Scleroscope.

The minimum hardness should prevail at 2/3 of journal circumference.

Hardening

Journals without hardened fillets can be inductionhardened or flame-hardened. Journals with hardened fillets (arrow) should be induction-hardened on principle. If this is not possible, scrap crankshaft.

Checking and reconditioning of crankshaft – rysunek

When hardening journals without hardened fillets, the distance A between runout of hardened surface and fillet (4–5 mm) must be maintained.

Checking the hardening

For perfect hardening, check adjustment of hardening equipment by metallographic grinding.

Pertinent tests can be made on scrapped crankshafts.

Check hardening by etching the journal surface with a 2% alcoholic nitric acid (HNO3) solution.

No dark spots should show up at surface of journal.

Non-hardened fillets will become dark.

The hardened fillets, on the other hand, should be as bright as the journal surface.

For comparison, we recommend an etching test on a metallographically inspected journal.

Then, carefully wash off nitric acid by means of alcohol.

Corrosion protection

Coat crankshafts which are not immediately installed again with engine initial operation oil (SAE 30).